VACUUM FORMED SHAPES are produced by dewatering a slurry of BULK FIBER and high-temperature binders. This manufacturing method permits considerable freedom to vary shape and thickness.
Please do not hesitate to contact us if you are concerned about smoke or smell during the initial heat-up.
For more information on RCF Free Vacuum Formed Shapes (Alkaline Earth Silicate wool), please contact us.
FIBERMAX | VFS | VFS | VFS | VFS | |
15P | 16P | 17P | 18R | ||
Color | White | White | White | White | |
Max. Service Temperature (℃) | 1500 | 1600 | 1700 | 1800 | |
Bulk Density (kg/m³) | 230 | 300 | 350 | 450 | |
Modulus of Rupture (MPa) | room temperature | 0.50 | 0.6 | 1.11 | 1.10 |
after firing at 1500℃×24hrs | 0.24 | – | – | – | |
after firing at 1800℃×24hrs | – | – | – | 0.73 | |
Linear Shrinkage (%) | 1300℃×24hrs | 0.4 | – | – | – |
1400℃×24hrs | 0.6 | 0.5 | – | – | |
1500℃×24hrs | 0.2 | -0.2 | 0.0 | – | |
1600℃×24hrs | – | -0.2 | -0.1 | – | |
1700℃×24hrs | – | – | 0.4 | -0.5 | |
1800℃×24hrs | – | – | – | 0.7 | |
Thermal Conductivity (W/(m・K)) | at 800℃ | – | – | – | 0.18 |
at 1000℃ | 0.24 | 0.23 | 0.21 | 0.23 | |
at 1200℃ | 0.28 | 0.27 | 0.25 | – | |
at 1300℃ | – | – | – | 0.34 | |
at 1400℃ | 0.34 | 0.32 | 0.30 | 0.34 | |
Loss on Ignition (%) | 4 | 4 | 4 | 4 | |
Chemical Composition (%) | Al₂O₃ | 74 | 79 | 78 | 85 |
SiO₂ | 26 | 21 | 22 | 15 | |
Firing Treatment | Yes | Yes | Yes | Yes |